The collage of an EPDM sheet
Training report dedicated to the assembly of EPDM membranes with primary and junction strip. The products and characteristics cited are those of the reportage.
The vulcanization of an EPDM tarpaulin is an expression that scares many people, and yet... By following a few basic rules, it all becomes childish simplicity. I was lucky to have been able to participate in a training given by Firestone on the techniques of collage and folding of EPDM tarp.
I particularly thank Eliane, Dominique and Jean-Claude des Eaux de la Mulle, without whom I would never have been able to attend this course. Also a big thank you to Ivan from Verhaert and the Firestone trainers who allowed me to make this report.
Before I get to the heart of the subject, I suggest a little bit of theory.
First question: what is EPDM? The answer is: rubber, simple rubber. Of course, not that of trees, but of synthetic rubber. This type of rubber is used both in the automotive industry (joints of windows, durites, ...) and in the construction (seam of windows, platforms, ...).
The characteristics of EPDM
- Elasticity: > 350 % (It is no longer elastic at -60°C, but without breaking)
- Sealing resistance: Resist 220 tons per square metre.
- UV resistance (This is the most important)
Tests were carried out on tarpaulins placed 20 years ago. As a result, they still have 150% elasticity. It is estimated that the life of the EPDM at, about, 70 years... Let's start the collage course.
Prepare the assembly of two sheets
To succeed correctly a vulcanization, you simply have to respect some golden rules:
1°) Do not be pressed. 2°) Prepare the support well. It must be very clean. No mud, soil, dead leaves, ... 3°) Be precise in the tracing of marker marks.
Collage material
QuickPrime Plus. This is the primary adhesion.
A QuickScrubber. It is the applicator buffer of the QuickPrime. This one is a kind of sponge to scour.
A roll of QuickSeam. It is the seal seal of the bonding.
Trace markers and position tarpaulins
The first step is to trace the tarpaulin from the bottom. Make a line every 15 cm from the edge of the tarpaline. Indeed, in order to have a good bonding, the tarpare from the top must cover the tarpain from below 15 cm. If there is more, it is not serious.
Then place the tarpaulin on top, just against its features.

Once the tarpaulin is well positioned, draw a line on the bottom tarpaulin every 30cm to 1cm from the edge of the top tarpaulin. These lines will later be used for the correct positioning of the seal.
Be very conscientious in this step as it is essential to get a waterproof bonding.

Then fold the top sheet on itself. It still has to cover the bottom sheet by ± 2cm. This so as not to collect soil when applying the primary.

Once this is done, draw a line (with the bonding primary) inside the fold of the top sheet in order to keep the sheet in place in case of a wind blow.
Don't worry about the tarpaulin, without the seal, vulcanization cannot be done.

Apply the primary and let it dry
Application of primary education
Dip the buffer into the primary. Let it drain. Turn the pad around so that it is well soaked from the primary. You can with this, clean and coat with glue 1 meter. Do not hesitate to pass the edge of the top sheet and the reminder lines when applying the primary.

To properly apply the primary, start with the outer edge of the tarpaulin and make 2 go back by pressing. You must feel the tampon scratching the tarp.

We arrive at the most pleasant part: we must let the primary dry.
So we're not doing anything.
Set the junction strip
The primary is dry... it's time to move on to the joint laying.
This is where the 30cm spacing marks will serve us.
Place the seal roll on the 3rd mark. The edge of the roller faces you inside the marks and just against the mark.

Roll it to the edge of the tarpaulin, passing it by a small centimeter.
Place the joint with the hand from the edge of the sheet towards the roll. Without pressing too hard, simply place the seal.

You move the roll three marks further, you place the joint on the tarpaulin and so on.

Tip: If, for some reason or another, you're deviating marks, never try to get the line back. Stop, cut the joint, put a little primary at that place, and go back from there, as at the beginning. If you don't do this, you take the big risk of having a very small fold, and therefore, not having any more sealing.
When you reach the end, cut the joint 1cm from the edge and continue.

Maroufling the Band
The next operation is to muffle the joint in the direction of length. Here, do not be afraid to press well. Try not to have air bubbles between the joint and the tarpaulin.

Drop the tarp and remove the protective paper
Once the joint is well muffled, allow the top sheet to be placed on the joint.
Do not remove the protective paper from the seal yet. This step will take place later.


Remove the protective paper by making a 90° angle to the tarpaulin.
Simply place the top sheet without pressing the joint. Do this with the hand, starting from the outside of the sheet to the inside.

Finishing the marouflage
It's done... okay.
Now, you're poking the top sheet perpendicularly, always from inside to outside.
Once it's done, you smear parallel to the tarpaulins.
We're done. If you have complied with the above instructions, here's what you should get: one perfectly waterproof tarpaulin.